CR SDC is a general purpose sulfur modified polychloroprene rubber having slow to medium rate of crystallization and medium mooney. Being a sulfur modified polymer is has superior bonding properties to metal, fabric, etc.
| Properties | Nominal Value |
| Form | Chips |
| Colour | Light Brown |
| Mooney Viscosity (ML 1+4 @ 100°C) | 45 +/-10 MU |
| Crystallization Rate | Medium to Slow |
| Specific Gravity | 1.23+/-0.02 |
| CR SDC | 100 |
|---|---|
| Qureacc® MBTS | 0.5 |
| Mgo(Starmag®150) | 4 |
| Stearic Acid | 1 |
| FEF N-550 | 60 |
| DOP | 10 |
| Zinc Oxide | 5 |
Physical Properties- Cure Time 10min @160°C | |
| Hardness(Shore A) | 70 |
| Tensile Strength(MPa) | 16.5 |
| Elongation at Break( %) | 450 |